Why our sea glass glaze crawls, and how we fixed it
Three batches, a lot of test tiles and one honest spreadsheet. What went wrong with the studio's newest glaze, and the two small changes that saved it.
When we mixed sea glass for the first time in January, everyone loved the test tiles. Soft green, a little cloudy where it pooled, like something you'd find on a beach after a storm. Then members started glazing real pots, and about one in four came out of the kiln with bald patches where the glaze had pulled back from the clay.
That pulling back is called crawling. It's one of the most common glaze faults, and it nearly always comes from one of three things.
The usual suspects
- Dust or grease on the bisque, so the glaze never grips.
- Too thick a coat, which cracks as it dries and then shrinks apart in the firing.
- A glaze that shrinks a lot as it dries, usually because of raw clay in the recipe.
We wiped down every bisque piece with a damp sponge for a week. The crawling barely changed, so dust was not our problem.
The tiles were dipped for two seconds. Members were dipping for five, because the glaze looked thin in the bucket.from the firing log, 14 February
Two small changes
First, we added a line to the glaze kitchen wall: dip for a slow count of two, no more. The bucket looks thin because it's meant to. Second, we swapped a little of the raw clay in the recipe for calcined clay, which has already shrunk and won't pull apart as it dries.
Batch three went into kiln two on a Saturday with a slower cool overnight. Out of 38 pots, one crawled, and that one had been dipped twice.
If you want to test it yourself
There are spare tiles on the shelf under the window. Note your dip time on the back in pencil and leave them on the cart. We'll fire them on Thursday and add them to the log.
Glaze with us
Members get the glaze kitchen, a test tile every week and a seat at the monthly glaze night.
See membership